Cast iron is one of the few materials where the cutting method decides the metallurgy of the finished part. Abrasive wheels and friction saws push heat into the workpiece; on grey iron that heat is mostly harmless, but on white or chilled iron it can provoke micro-cracking at the cut edge that only shows up after machining. Diamond wire removes material by grinding at low force with a narrow kerf, so the bulk of the part never sees a temperature rise.
The free graphite in grey iron acts as a built-in lubricant, which is why it machines easily — and also why it cuts inconsistently on wire. The graphite flakes interrupt the chip, so the wire alternates between cutting metal and sliding through soft graphite. The practical effect is a cut that runs fast but leaves a slightly ragged edge on thin sections.
White cast iron and chilled surfaces are the opposite problem. They contain cementite rather than free graphite, and hardness commonly runs from 400 to 600 HB, with some chilled rolls and mill liners going higher. These are the grades where abrasive saws slow down badly and where diamond wire earns its cost.
| Workpiece | Wire diameter | Diamond grit | Bond |
|---|---|---|---|
| Grey iron, section under 100 mm | 0.25–0.30 mm | #80–#120 | Nickel-plated |
| Grey iron, heavy section | 0.35–0.45 mm | #40–#60 | Nickel-plated |
| White / chilled iron | 0.30–0.40 mm | #40–#80 | Nickel-plated, high density |
| Thin-wall castings, minimal kerf | 0.20–0.25 mm | #120–#150 | Nickel-plated |
Finer grit gives a cleaner edge but cuts slower and loads more easily in the graphite. On mixed batches, it is usually cheaper to run one coarse wire and accept a slightly rougher edge than to change spools between parts.
On grey iron, wire speed typically sits in the 15–25 m/s band with a light feed; the wire should be cutting, not rubbing. On chilled iron, drop the speed and keep the tension steady rather than pushing the feed, because the failure mode there is diamond pull-out, not wire breakage. Use a water-based coolant with a rust inhibitor — cast iron will flash-rust on the cut face within hours if it is left wet.
These are starting points, not settings. Section thickness, casting skin and the amount of sand inclusion all shift the window, and the only reliable way to fix a parameter set is a test cut on your own material.
We keep test results on grey, ductile, white and chilled iron, and we will tell you which wire we would run and what it should cost per square metre of cut. If a different process suits your part better, we will say so.
Send us a sample of your material. We return a cut-quality report with the wire specification and machine format that suit it — free of charge, no obligation.
ENSOLLTECH PTE. LTD. · Singapore (UEN 202551184N) · manufacturing in Zhengzhou, China · reply within one working day
Not listed? Send a sample and we will cut it and tell you what wire to run.
Supplied by ENSOLLTECH PTE. LTD.
ENSOLLTECH PTE. LTD. is a Singapore company (UEN 202551184N), registered at 266A South Bridge Road, #02-01, Singapore 058815. We supply endless diamond wire loops and diamond wire saw machines; the products are manufactured at our group’s own ISO 9001-certified plant in Zhengzhou, China — not sourced from third-party traders.
Company profile: About ENSOLLTECH · Technical enquiry: Contact our Singapore office
If you have any question, please contact us